A buyer received a plating report that read 0.25 micron on the face of a pendant and 0.09 micron at the edge of the bail. The supplier had quoted 0.25 micron and met it at the point that was measured. The dispute was not about lying; it was about where the measurement happened.

Plating thickness is the number that decides a replating claim, and it is the number most orders leave unmeasured. Measuring it, and specifying where it counts, removes most plating arguments before they start.
Why thickness varies across a piece
Electroplating deposits metal according to current density. Current concentrates at edges, corners and high points, and it thins in recesses and on large flat areas.
The edge effect
An edge can carry two to three times the current density of a flat face, which deposits a thicker layer in some baths and a thinner, burnt layer in others. The result is that a piece plated to 0.15 micron on the face may show 0.10 at an edge or 0.22, depending on the bath and the rack.
The recess effect
Recesses receive less current and therefore less metal. A groove or a milgrain detail is often the thinnest point on the piece, and it is also a place where tarnish starts because the plate is incomplete.
Why the bail reading in the opening example was low
A bail is a small curved form with a large surface area relative to its size. It sits at the edge of the rack's throwing power, and it reads low on almost every plated pendant. That is a design and racking issue, not a bath failure.
Test methods and what each is for
Three methods cover most needs, and they differ in speed, cost and what they can tell you.
| Method | Destructive | Best use |
|---|---|---|
| X-ray fluorescence | No | Routine check, incoming inspection |
| Cross section | Yes | Disputes, layer structure |
| Coulometric stripping | Yes, local | Single layer thickness, lab |
XRF is the workhorse. A handheld unit reads a spot in seconds and needs no sample preparation, so it can be used on finished pieces at incoming inspection. Its limitation is that it reads an average over the spot, which flattens the variation you may be trying to see.
Cross section for disputes
Mounting the piece, polishing a section and measuring the layer under a microscope gives the layer thickness and its structure. It destroys one piece and it settles an argument that XRF cannot, because it shows whether the plate is continuous.
Coulometric stripping
Anodic stripping removes the layer in a controlled way and measures the charge, which gives thickness for a known area. It is a laboratory method and it is used for specification verification rather than for production.
Where to measure
A single reading is not a thickness specification. Three points give a usable picture.
- Flat face: the highest reading on most pieces
- Shank edge or rim: the wear zone and usually the lowest reading
- High point such as a prong tip or bead: the contact zone
Record all three and specify the minimum at the edge. A specification of 0.15 micron at the edge implies a face reading of 0.18 to 0.25, which is what most buyers actually want.
Sample size
Five pieces per batch for a routine check, and twenty for a first order or a new supplier. Plating varies across a rack, so sampling from one position understates the variation; take pieces from the front, middle and back of the rack.
Writing a specification a supplier can meet
A specification has four parts: metal, thickness, measurement point and tolerance. Missing any one of them leaves room for a different reading.
Metal and sublayer
State the plating metal and any sublayer, such as a palladium strike or a nickel barrier. A rhodium layer over silver behaves differently from rhodium over a nickel barrier, and the barrier affects tarnish resistance.
Thickness and point
State the number and the point: 0.15 micron minimum at the shank edge, measured by XRF. A number without a point is a target, not a specification.
Tolerance and testing frequency
Plus or minus 20 percent, tested on five pieces per batch and twenty on the first order. Add the requirement that the supplier reports the readings with the shipment.
Reading a supplier's report
A plating report is a document to read critically, not to file. Three details decide whether it means anything.
Where was the reading taken
A report that states a single number without a point is a report that measures the easiest place. Ask for the point, and compare it with the wear zone you care about.
How many pieces
A report on one piece describes one piece. A report on five from different rack positions describes a batch.
What instrument
XRF, cross section or stripping all produce numbers that are not directly comparable. A change of method between orders can look like a change in quality when nothing changed in the bath.
Putting thickness into the cost conversation
Plating thickness is a cost line, and it is a small one relative to the service it prevents.
Moving from 0.10 to 0.15 micron adds a fraction of a dollar per piece at volume. It roughly doubles the interval before visible wear, which removes a replating service and a customer conversation from the first year of ownership.
Where thicker plating costs more than it saves
Above 0.30 micron the deposit can crack at sharp edges, and the crack becomes a corrosion site. A very thick plate also looks slightly milky on silver, which reads as lower quality under a display light. The useful ceiling is around 0.30 micron unless the piece is designed for it.
What our plating terms include
We plate white metal at 0.15 micron minimum at the edge, measured by XRF, and report the readings with the packing list. A 0.25 micron option is available for warranty programmes with a stated service interval.
Minimum order is 50 pieces per design. Stock ships in three to five days and bulk in fifteen to twenty days under 500 pieces. Payment is a 30 percent deposit with the balance before shipment, by T/T, PayPal or Western Union. Samples ship with the thickness report so the first order can be checked against a known reading.
Common plating defects and their readings
The thickness reading usually explains the defect, and the pattern of readings points at the bath or the racking.
Patchy colour
A patch that reads thin at one point and full at another is a current density problem, often from poor racking or a contact fault. The fix is racking and contact maintenance, not more plating time.
Blistering and peeling
Peeling usually comes from surface preparation rather than thickness. A plate that peels reads correctly for thickness and fails in adhesion, which no thickness gauge will show.
Milky appearance
A milky look on a thick plate is a brightness problem in the bath, usually from organic contamination. It reads as a colour defect and it is a chemistry defect.
Dark edge
A dark rim at a sharp edge is a burnt deposit from excessive current density at the corner. It reads thicker at the edge, which is the opposite of the wear problem and the same root cause: current concentration.
When to re-measure
Re-measure after any change that could move the deposit: a new bath, a new rack, a new plater, a new shape. A change of shape matters more than most buyers expect, because a bail or a narrow band sits differently in the current field.
Re-measure also after a complaint. A complaint with no reading is a conversation about impressions, and a complaint with a reading is a decision about rework.
Frequently Asked Questions
Can I measure plating on a stone-set piece?
Yes on the metal, avoiding the stones. XRF reads the metal beneath the spot, so a reading taken over a stone gives the stone's composition rather than the plate.
Does plating thickness affect colour?
It affects brightness more than hue. A very thin plate lets the warmer silver show through at the edges, which reads as a colour difference even when the bath is correct.
How often should a programme test?
Every batch for the first three orders with a new supplier, then quarterly with five pieces per batch. A supplier whose process is stable will pass; one whose process drifts will show it in the quarterly check.
Is gold plating measured the same way?
Yes, with the same instruments. Gold is softer, so the wear interval at a given thickness is shorter than rhodium, and a 0.15 micron gold layer typically shows wear before a 0.15 micron rhodium layer does.
Next step
Ask for a thickness report with measurement points on your next sample order, and add the three point requirement to your specification. Our production desk supplies the report, and the guide index covers the replating interval that follows from it.